Monday, November 16, 2009
Cotfix RR series
Textile Testings - Testing the purity of Acetic Acid
The strength of acetic acid may be easily and accurately tested by finding the freezing point of acetic acid. Since acetic acid may easily be adulterated with some strong acid to give the required acid strength (if tested by usual acidimetric titration), it always better test any one its physical property. The freezing point of Glacial Acetic acid (98 to 100%) is 16.7°C. If the test sample freezes below 16.7°C, then we could fix that the acid is adulterated with water and the strength will be lower than Glacial acetic acid. On the other hand if the freezing point is higher than 16.7°C, some other acid admixture would have changed it and in this case also it is not pure. So while testing the acid strength, we could allow a maximum deviation limit of +/- 5% from the freezing point for some instrumental errors.
Testing Procedure:

1. Attach a test tube clamp to the ring stand so the tube is about 25cms above the base. Place the test tube in the clamp near the top of the tube and tighten the clamp securely.
2. Place a thermometer in the slotted cork so that the temperature scale is visible through the slot. Position the cork so that the thermometer is about 1 cm from the bottom of the test tube when the cork is place as shown in the figure.
3. Measure 10ml of pure acetic acid using a graduated cylinder. Pour the acid into the test tube and replace the thermometer.
4. Adjust the temperature of acetic acid to about 25°C by warming or cooling the test tube in beaker of water (with or without ice cubes).
5. Empty the beaker and fill it with ¾ with crushed ice. Add cold water until the ice is almost covered. Place the beaker of ice water below the test tube assembly.
6. Carefully read the thermometer and record the temperature as the 0 minute reading in a data table.
7. Lower the test tube assembly in to the ice water beaker. Be sure to lower the test tube until all of the acetic acid is under water. Refasten the clamp to the ring stand.
8. Loosen the cork slightly and agitate the acetic acid slightly using the thermometer. Be careful not to bang the thermometer bulb on the glass and keep the thermometer bulb completely immersed in the acid. Take temperature reading every 30 seconds as the acid cools. Begin with the 0.5 minute reading.
9. Stop stirring the acid as soon as you are sure the crystals are forming. Keep taking readings until a total of 15 minutes as passed. Stir the ice water occasionally to help it at a constant temperature.
10. After completing the temperature readings remove the test tube assembly from the water. Replace the ice water in the beaker with warm water. Immerse the test tube assembly in the warm water and begin taking temperature readings every thirty seconds as the acetic acid melts. Once the acid has melted a little and moves easily in the test tube agitate the solid mixture with the thermometer. Continue taking readings until all the acetic acid is melted.
Conclusions:
1. Draw a smooth curve using the readings. Time vs temperature.
2. From this data we can find out the freezing point and melting point of acetic acid. Infer that if it is close to 16.7°C, then it is a pure acid.
Saturday, November 14, 2009
Viscose Rayon Pretreatment -Knitted fabric
Scouring (No bleaching for dark and medium shades):
* 2 – 4 ml/l Lubricating agents
* 0.5 – 1 g/l Wetting & scouring agent
* 0.5 – 2 g/l Chelating agent
* 1.0 - 3.0 g/l Soda ash
o Run 20 to 30 minutes at 60-90° C
o Hot wash
Peroxide bleach on jet or overflow machine
For full white
1.0 – 3 ml/l Lubricant
2 – 4 g/l Optical Whitener
2 – 6 ml/l Hydrogen peroxide 35%
0.3 – 0.7 % Peroxide Stabilizer
* Run 40 minutes at 85° C
* Hot rinse at 60 – 80° C
* Neutralise with core acid neutralizer for 10 – 15 minutes at 50-60° C
Note: There is a high risk of forming permanent creases in rope dyeing machines because viscose fibre swells and fabrics become stiff. Fabric will therefore not run well at temperatures below 50° C. Fabric must always be run at temperatures of 50° C or higher. Cool at a gradient of not more than 1° C per minute to prevent hydro plastic creasing.
Viscose Rayon Pretreatment -woven fabric
Warps of viscose rayon can be sized with a variety of agents : starch based systems, polyvinyl alcohol systems or a combination of both, modified starch, starch ethers or CMC or combinations of these.
Desizing:
Identification of the size present is important prior to deciding on a suitable desizing procedure, however, many factories will opt to use their standard cotton desize treatment :
e.g. applying in the quench box of a singeing machine :
pad 2 - 4 g/l amylase enzyme
1 - 2 g/l wetting agent
impregnate at 60°C ; pick-up 80 % ; batch minimum 4 hours - normally
overnight ; wash-off.
Scouring & Bleaching:
Relax / scouring
Viscose rayon fibres, unlike natural cellulosic fibres, are free from natural fats and waxes, motes and seeds, and the scouring process, therefore, need not be as severe as for cotton, and can be based on soda ash or tetra sodium pyrophosphate recipes rather than caustic soda. A typical scouring recipe on a 5 box continuous open width washing range would be :
Box 1
3 g/l Wetting and scouring agent
2 g/l Soda Ash
1 g/l Sequestering/chelating agent
at 95°C
Box 2
1 g/l Sequestering/chelating agent at 95°C
Box 3
2 g/l Sequestering/chelating agent at 95°C
Box 4
Water only at 70°C
Box 5
Water only – cold
Causticising
Causticisation modifies the viscose fibre surface or skin to enable more rapid diffusion of dye into the fibre. Benefits are therefore more obvious in printing than in dyeing, where long diffusion times are employed, and with selected reactive dyes, yield gains of up to 50% are possible.
Typical conditions for pure viscose are treatment with 6° - 8° Bé caustic soda at 25° - 30° C for at least 2 minutes followed by low tension washing with boiling water to assist the rapid removal of alkali. Pad-Batch processing is popular although dedicated continuous plant, employing a scray or conveyor for tensionless swelling and reaction, is preferable. Liquor pick-up of about 120% should be achieved. The best after-washing device is probably a sieve drum continuous open-width range. Low uniform processing tensions are essential for consistent results and good quality. Rinsing should be done as hot as possible to minimise swelling and ensure rapid and complete removal of caustic soda.
An addition of 2 – 4 g/l soda ash in the initial wash boxes will promote removal of alkali, and help maintain a good fabric handle. Neutralisation with Core neutralizing agents, is also advisable.
Viscose Rayon Properties
Different ratio of crystalline and amorphous regions compared to cotton | Viscose has higher dye affinity than cotton. |
| Viscose has irregular serrated skin and cross section. | Inferior diffusion and penetration. More kinetic energy needed. Hot reactive dyes. |
| Viscose loses tenacity when wet. | More care needed to avoid damage. |
| Wet swelling increases with temperature | Very important in package dyeing. Liquor circulation should mainly be IN to OUT. OUT to IN should be <> |
| Swelling of fibres makes wet fabrics stiff. Swelling and heat can set creases. | Use longer L.R. than for cotton. Keep liquors above 50° C, Cool at maximum 1° C per min. Use suitable anti-crease lubricants. |
| Viscose may contain residues of sulphur. | Mild peroxide bleach may be necessary to remove sulphur. |
| Viscose is creamy white in colour, naturally clean. Fabrics free from natural fats and waxes, motes and seeds. | Little preparation required. Bleaching chemicals can be reduced. Always give SOME preparation to avoid carry over of sulphur. |
| Dyes have higher substantivity and faster fixation | Use ‘Migration’ dyeing techniques (at up to 110° C). Add salt after dye. |
Pretreatment of Viscose
- Scouring and bleaching need to be mild in nature. The fabrics should always be scoured, and never put straight into dye because it is important to remove any residual sulphur to prevent dye reduction. Spinning lubricants used on viscose tend to yellow with heat, and so should be removed for best whites and bright pastels.
- The liquor ratio may need to be a little higher than for cotton, because of the higher water retention but also because of the high swelling. (Reduce jet capacity).
- Break outs are always an issue on viscose, particularly where there is lengthways tension on the fabric. Best avoided by sewing the fabric at an angle, not straight across. Use multiple "zig-zag" stitching for additional security.
- Fabrics will tend to stiffen in tight constructions so lubrication is important. There should be as little tension on the fabric as possible, because of the low wet modulus it will stretch easily and dimensional stability may never be achieved. Usually means slower turn around times and dyeing machines with winches to help the fabric into the jet, or the cigar-type machines with the fabric movement into the jet being downwards (like the Gaston County Futura). The more “soft flow”the dyeing machine – the better.
Viscose Rayon Preparation
Viscose Rayon Preparation
Manufacturing of Viscose Rayon:
- Possible sulphur residues can generate reducing conditions – destroying or changing the shade of dyestuffs
- After initial skin formation, the core of the fibre decomposes, hardens and shrinks. Viscose fibres are therefore characterised by an irregular, serrated skin and cross section. The skin is said to consist of many small crystalline regions. The core, on the other hand, develops a coarser crystalline structure.
- Differences in the ratio of skin to core impact on fibre properties and dyeing behaviour. Dye diffusion is therefore
crucial to dyeing speed and extra kinetic energy is needed for dye penetration – especially when swollen to its maximum by heat.
Properties of Viscose:
- Viscose has lower tenacity in both wet and conditioned state than cotton – more care is necessary to prevent fabric breakages and tears in wet processing.
- Viscose has greater elongation in both wet and conditioned state than cotton – it will be stretched or distorted more under tension.
- Viscose and Modal fibres are supplied in a pure state and with a higher degree of whiteness than cotton. Bleaching is only required for a full white or pastel shades. Viscose/cotton blends require bleaching baths with a reduced chemical content.
- The water retention value (swelling index) of viscose is very much higher than that of cotton. In aqueous liquors, viscose fibres tend to swell more strongly than Modal fibres or cotton. This swelling process happens very quickly and is almost complete after ten seconds at the lower temperature range.
- Fabrics become much more stiff when wet because the fibres are so swollen. In their swollen state, viscose fibres can become set to a certain extent. This is called hydro plasticity.
Stages of Cotton Processing - III
Cotton Processing Flow Chart
Various stages of wet processing, shown in the above figure, involve treating greige goods with chemical baths and often additional washing, rinsing and drying steps. Some of these stages may be optional, depending on the style of fabric being manufactured or whether the material being wet-processed is a yarn, or a knitted or woven fabric.
Some of the key steps in the treatment of cotton material include singeing, desizing, scouring, bleaching, mercerizing, as well as dyeing and finishing.
Singeing is a dry process that removes fibres protruding from yarns or fabrics. Desizing is a wet process that removes the sizing material applied to the warp yarns before weaving. Scouring is a cleaning process that removes impurities from fibres, yarns or cloth through washing, usually with alkaline solutions. Bleaching is a chemical process that decolourizes coloured impurities that are not removed by scouring and prepares the cloth for further finishing processes such as dyeing or printing. Mercerization is a chemical process to increase dyeability, lustre and appearance. Dyeing operations are used at various stages of production to add colour to textiles and increase product value. Dyeing can be performed using batch or continuous processes. Common methods of batch or exhaust dyeing include package, beam, beck, winch, jet and jig processing. Continuous dyeing processes typically consist of dye application, dye fixation with chemicals or heat, and washing. Dyeing processes may take place at any of several stages of the manufacturing process (fibres, yarn, piece-dyeing). Stock dyeing is used to dye fibres; yarn dyeing is used to dye yarn; and piece/fabric dyeing is done after the yarn has been constructed into fabric. Printing is a localized or patternised coloration of the fabrics. Fabrics are printed with colour and patterns using a variety of techniques and machine types. Finishing encompasses chemical or mechanical treatments performed on fibre, yarn or fabric to improve appearance, texture, or performance.